The strongest filament: four ways to measure it
"Strongest" is four questions. To pull and to stay stiff, PPA-CF: 168 MPa tensile strength along the layers, 57 MPa across them and a 9,860 MPa bending modulus on Bambu Lab's datasheet, first on all three among the grades we print or order in. To take knocks along the layers, PAHT-CF or PC FR; across the layers, PA6-CF or PLA Basic. If the part may flex, a TPU beats all of them on impact. The rigid winners, PPA-CF, PAHT-CF and PA6-CF, all need a heated chamber and a hardened nozzle; we print them from one part and post to the Baltics, Finland, Sweden and Denmark.
- PPA-CF: 168 / 57 MPa tensile strength along / across the layers (ISO 527)
- Impact: PAHT-CF 57.5 kJ/m² along the layers, PA6-CF 15.5 across (ISO 179, unnotched)
- PPA-CF, PPS-CF, PET-CF and PC FR 2-5 working days after payment
- Heated-chamber grades up to 340 x 320 x 340 mm in one piece
Which filament is strongest for my part?
It depends on the load. To pull and to stay stiff: PPA-CF, 168 MPa along the layers. To take a knock along the layers: PAHT-CF at 57.5 kJ/m² unnotched, ordered in, or PC FR at 55. To take a knock across them: PA6-CF at 15.5 kJ/m², ordered in, or PLA Basic at 13.8 if the part stays cool.
If the part may bend, a bumper or a guard that takes hits, it is a TPU part.
Strong is four rows

A datasheet does not have a strength row. It has tensile strength (ISO 527), the stress at which a pulled bar breaks; bending modulus (ISO 178), how much a bar resists bending, which is stiffness, not strength; and impact strength (ISO 179), the energy a bar absorbs when struck, measured here on unnotched specimens. Each is given along the layers (X-Y) and across them (Z), and the Z figure is the one a printed part breaks at when the load is wrong.
None of these is a safety factor or a load rating for your part. Bambu Lab gives every figure "for design reference and comparison only", measured on its own specimens, and the specimens were not treated alike: PPA-CF and PPS-CF "were not annealed before testing"; PA6-CF, PAHT-CF and PC FR were annealed and dried at 80 °C for 12 hours; PETG HF at 75 °C for 8 hours; PLA Basic at 55 °C for 8 hours.
Tensile strength, every grade we print or order in
Ranked on tensile strength along the layers (ISO 527) from Bambu Lab's datasheets. "Kept across the layers" is derived: the Z figure divided by the X-Y figure. "Needs" is what the grade takes to print at all: a heated chamber (a recommended chamber of 45 °C or more, or an enclosure required) and a hardened nozzle (carbon or glass fibre). PLA Pure is listed but not ranked: its datasheet gives 51.5 MPa against PLA Basic's 35 while Bambu Lab says the two match in mechanical performance, so we compare those two on bending, not on this row.
| Tensile strength X-Y / Z (ISO 527) | Kept across the layers | Elongation at break X-Y (ISO 527) | Needs | Our status | |
|---|---|---|---|---|---|
| 1. PPA-CF | Tensile strength X-Y / Z (ISO 527)168 / 57 MPa | Kept across the layers34% | Elongation at break X-Y (ISO 527)3.2% | Needsheated chamber, hardened nozzle | Our statusmost popular |
| 2. PA6-CF | Tensile strength X-Y / Z (ISO 527)102 / 48 MPa | Kept across the layers47% | Elongation at break X-Y (ISO 527)5.8% | Needsheated chamber, hardened nozzle | Our statusordered in |
| 3. PAHT-CF | Tensile strength X-Y / Z (ISO 527)92 / 47 MPa | Kept across the layers51% | Elongation at break X-Y (ISO 527)8.4% | Needsheated chamber, hardened nozzle | Our statusordered in |
| 4. PPS-CF | Tensile strength X-Y / Z (ISO 527)87 / 24 MPa | Kept across the layers28% | Elongation at break X-Y (ISO 527)1.2% | Needsheated chamber, hardened nozzle | Our statusmost popular |
| 5. PA6-GF | Tensile strength X-Y / Z (ISO 527)75 / 27 MPa | Kept across the layers36% | Elongation at break X-Y (ISO 527)3.9% | Needsheated chamber, hardened nozzle | Our statusordered in |
| 6. PET-CF | Tensile strength X-Y / Z (ISO 527)74 / 35 MPa | Kept across the layers47% | Elongation at break X-Y (ISO 527)4.5% | Needsheated chamber, hardened nozzle | Our statusmost popular |
| 7. PC FR | Tensile strength X-Y / Z (ISO 527)60 / 21 MPa | Kept across the layers35% | Elongation at break X-Y (ISO 527)2.4% | Needsheated chamber | Our statusmost popular |
| 8. PC | Tensile strength X-Y / Z (ISO 527)55 / 34 MPa | Kept across the layers62% | Elongation at break X-Y (ISO 527)3.8% | Needsheated chamber | Our statusordered in |
| 9. PLA-CF | Tensile strength X-Y / Z (ISO 527)38 / 26 MPa | Kept across the layers68% | Elongation at break X-Y (ISO 527)8.4% | Needshardened nozzle | Our statusordered in |
| 10. ASA | Tensile strength X-Y / Z (ISO 527)37 / 31 MPa | Kept across the layers84% | Elongation at break X-Y (ISO 527)9.2% | Needsheated chamber | Our statusordered in |
| 11. ABS-GF | Tensile strength X-Y / Z (ISO 527)36 / 29 MPa | Kept across the layers81% | Elongation at break X-Y (ISO 527)6.3% | Needsheated chamber, hardened nozzle | Our statusask |
| 12. PLA Basic | Tensile strength X-Y / Z (ISO 527)35 / 31 MPa | Kept across the layers89% | Elongation at break X-Y (ISO 527)12.2% | Needsneither | Our statusmost popular |
| 12. PETG-CF | Tensile strength X-Y / Z (ISO 527)35 / 29 MPa | Kept across the layers83% | Elongation at break X-Y (ISO 527)10.4% | Needshardened nozzle | Our statusordered in |
| 14. ASA-CF | Tensile strength X-Y / Z (ISO 527)34 / 30 MPa | Kept across the layers88% | Elongation at break X-Y (ISO 527)9.6% | Needsheated chamber, hardened nozzle | Our statusordered in |
| 14. PETG HF | Tensile strength X-Y / Z (ISO 527)34 / 23 MPa | Kept across the layers68% | Elongation at break X-Y (ISO 527)8.6% | Needsneither | Our statusmost popular |
| 16. ABS | Tensile strength X-Y / Z (ISO 527)33 / 28 MPa | Kept across the layers85% | Elongation at break X-Y (ISO 527)10.5% | Needsheated chamber | Our statusordered in |
| 17. ASA Aero | Tensile strength X-Y / Z (ISO 527)32 / 21 MPa | Kept across the layers66% | Elongation at break X-Y (ISO 527)5.1% | Needsheated chamber | Our statusmost popular |
| PLA Pure (not ranked) | Tensile strength X-Y / Z (ISO 527)51.5 / 30.0 MPa | Kept across the layers58% | Elongation at break X-Y (ISO 527)5.6% | Needsneither | Our statusordered in |
| TPU 95A HF | Tensile strength X-Y / Z (ISO 527)27.3 / 22.3 MPa | Kept across the layers82% | Elongation at break X-Y (ISO 527)more than 650% | Needsneither | Our statusordered in |
| TPU for AMS | Tensile strength X-Y / Z (ISO 527)22.4 / 11.2 MPa | Kept across the layers50% | Elongation at break X-Y (ISO 527)more than 650% | Needsneither | Our statusmost popular |
| TPU 90A | Tensile strength X-Y / Z (ISO 527)12.5 / 10.1 MPa | Kept across the layers81% | Elongation at break X-Y (ISO 527)more than 650% | Needsneither | Our statusordered in |
| TPU 85A | Tensile strength X-Y / Z (ISO 527)12.0 / 10.5 MPa | Kept across the layers88% | Elongation at break X-Y (ISO 527)more than 700% | Needsneither | Our statusordered in |
The working for the third column: PPA-CF 57 / 168 = 0.34, so 34%. Read it with the tensile figures: PPA-CF is first both ways, 168 along the layers and 57 across, yet it keeps only a third of its strength across them, while PLA Basic keeps 89% of a much smaller number. Below the top eight the ranked rigid grades sit between 32 and 38 MPa along the layers; for most of the catalogue, "strong" is decided by the other rows.
The TPU grades are at the bottom on tensile strength and at the top on impact along the layers, which is the point of the next section: one row never answers the question.
The winner of each way
- To pull: PPA-CF168 MPa along the layers and 57 MPa across them (ISO 527), first on both. PA6-CF follows at 102 / 48 and PAHT-CF at 92 / 47, both ordered in. PPA-CF, PPS-CF and PET-CF are on our most popular list. When a buyer writes "the strongest you have", this is the row that answers it.
- To stay stiff: PPA-CFBending modulus 9,860 MPa along the layers (ISO 178), then PPS-CF 7,160, PA6-CF 5,460 and PET-CF 5,320. Across the layers PPA-CF keeps 3,240 MPa. Stiffness is what a bracket, an arm or a plate that must not flex needs; it is not the same as strength, and a stiff grade is often a brittle one: PPA-CF breaks at 3.2% elongation, PPS-CF at 1.2%.
- To take a knock along the layers: PAHT-CF, then PC FRUnnotched impact strength (ISO 179, X-Y) among the rigid grades: PAHT-CF 57.5 kJ/m², ordered in; PC FR 55, on our most popular list; PPA-CF 41.7. Notched, where a sharp corner starts the crack, the order changes: PAHT-CF 22.8, ABS 21.5, ASA 19.6. Any TPU grade reaches 123.2 to 124.3 unnotched if the part may flex.
- To take a knock across the layers: PA6-CF, then PLA BasicUnnotched impact strength in Z among the rigid grades: PA6-CF 15.5 kJ/m², ordered in; PLA Basic 13.8, on our most popular list; PAHT-CF 13.3. The carbon-fibre grades on our most popular list give 2.8 to 4.5 here, so a part that is hit across its layers is designed so the hit runs along them, or printed in PA6-CF, PLA Basic or a TPU (86.3 to 88.5 kJ/m² for TPU 95A HF, 90A and 85A). The full X-Y against Z table for 12 grades is on Layer strength: X-Y vs Z.
Why the winners need a heated chamber
PPA-CF prints at 280-310 °C in a chamber of 50-80 °C, with a hardened steel nozzle that Bambu Lab calls "mandatory", after 8 to 12 hours of drying at 100-140 °C in a blast drying oven. PAHT-CF and PA6-CF want a 45-60 °C chamber, a hardened nozzle and 8 to 12 hours at 80 °C. PC FR wants a 45-60 °C chamber and 8 hours at 80 °C. These are the datasheets' own printing settings.
Bambu Lab says so itself. It printed its PPA-CF specimens with the chamber at 52 °C and writes: "If higher chamber temperature were used (i.g., 70 - 80 °C), higher mechanical properties would be obtained, especially the Z- direction's." For PPS-CF, printed at 60 °C: "If higher chamber temperature and nozzle temperature were used (i.g., 90 °C and 335 °C), higher mechanical properties would be obtained, especially the Z-direction's." In the maker's own words, a hotter chamber gives higher figures, most of all across the layers.
We print these grades in a heated chamber, which caps a part at 340 x 320 x 340 mm in one piece. What we do not claim is that our parts reach or beat the datasheet: Bambu Lab's figures are its specimens under its conditions, and ours are printed parts under yours.
Without a heated chamber
Seven of the grades we print or order in need neither a heated chamber nor a hardened nozzle: PLA Basic, PLA Pure, PETG HF and the four TPU grades. On comparable figures the strongest of them is PLA Basic, 35 MPa along the layers and 31 across (ISO 527), with PETG HF next at 34 / 23. PLA Basic also keeps the most across the layers of any rigid grade, 89%, and takes a knock there better than every carbon-fibre grade on our most popular list, 13.8 against 2.8 to 4.5 kJ/m².
So if the question is "the strongest filament my printer can print" and the printer has neither a heated chamber nor a hardened nozzle, the answer is PLA Basic for a cool part and PETG HF for a part that gets warm, PLA Basic's heat deflection being 54 °C at 1.8 MPa and PETG HF's 62 °C (ISO 75). The grades above them in the table are the ones we print; send the file.
Before you go to the strongest grade
About 30% of the enquiries we get name a material unprompted, and "the strongest you have" is one of the phrases; the rest describe where the part sits and what it does. Both work, and the second is often more useful, because the strongest grade is not always the right answer. We choose the print orientation, and the layer direction matters for strength; we add walls where the part carries load. A PETG HF part laid so the load runs along its layers, with thicker walls, can be the answer to a question that arrived as "strongest".
Two cases where no grade on the list fixes the design. A part loaded the same in every direction always has a weak direction in FDM, the Z axis, and the Layer strength guide says which grades keep the most of it. And a part that must be both stiff and take hits across the layers is asking for two winners at once; say which matters more, and a person picks.
What we print
PPA-CF, PPS-CF, PET-CF, PC FR, ASA Aero, PLA Basic, PETG HF and TPU for AMS are among our most popular materials, usually 2-5 working days after payment. The grades marked "ordered in" are ordered in for the job; the quote gives the time. Ask for two grades in one request and the quote prices each.
Largest part in one piece: 340 x 320 x 340 mm in every material. Tolerance ±0.5%, minimum ±0.5 mm. Posted to the Baltics, Finland, Sweden and Denmark.
Questions
Checked by the druckworks workshopUpdated
What is the strongest filament?
Of the grades we print or order in, on Bambu Lab's datasheets: PPA-CF on tensile strength (168 MPa along the layers, 57 across) and on stiffness (9,860 MPa bending modulus). On impact the winners are different: PAHT-CF along the layers, PA6-CF across them, and, if the part may flex, TPU: along the layers any TPU grade, across them TPU 95A HF, 90A and 85A.
Is carbon fibre always stronger?
No. Across the layers PPS-CF breaks at 24 MPa and PLA Basic at 31 (ISO 527), and on impact across the layers PPA-CF gives 4.3 kJ/m² against PLA Basic's 13.8 (ISO 179). PPA-CF is first on tensile strength both ways and on stiffness; the part has to be laid so the load runs along the layers.
What is the strongest filament without a heated chamber?
Without a heated chamber or a hardened nozzle, and on comparable figures: PLA Basic, 35 MPa along the layers and 31 across (ISO 527), then PETG HF at 34 / 23. Everything above them in the table needs a heated chamber, a hardened nozzle or both; those are the grades we print.
Is PETG stronger than PLA?
Along the layers they tie at 34 and 35 MPa; across them PLA Basic leads, 31 against 23. PETG HF takes more heat. The full comparison is on PETG or PLA for functional parts.
How does PPA-CF compare with metal?
We make no metal parts and this page makes no metal comparison. The page that does, with the stiffness gap in datasheet figures, is Carbon fibre vs aluminium.
Can you print PPA-CF from one part?
Yes. It is on our most popular list, usually 2-5 working days after payment, up to 340 x 320 x 340 mm in one piece.
How big can the strongest part be?
340 x 320 x 340 mm in every material.
Send the file and say where the load goes
Send the file and write which way the part is pulled, bent or hit. A person picks the grade and the print orientation and replies with a price in 3 hours on average on workdays.